BULLSEYE Billet 0843-65 F

transparent opalline


Abmessung 13 x 25 x 2 cm

Gewicht 1,54 kg


Bullseye Artikelnummer: 000843-0065-F-EACH


0843 Opaline Casting Tint Billet

Opaline Casting Tint Billet (000843-0065-F) only reveals its rich and varied color range through a unique firing process. When viewed at process temperature during the casting firing, Opaline Casting Tint will appear colorless and clear. If allowed to cool and anneal as you would other styles, it will remain colorless. To develop Opaline Casting Tint's unique color during a single casting firing, the following striking process must be followed:


Striking Instructions

Cast the glass and perform any anti-sucker* holds needed, then cool to 538 °C, and hold it there for at least 1:00 to unify the temperature throughout the glass. If casting a form that is thicker than 25mm, hold for at least 1 hour per 25mm of thickness. The thicker the glass, the longer it will need to be held at 538 °C to unify the temperature.

Next, reheat to 663 °C to develop color. The saturation of color and degree of opalescence that develop depend on how long the glass is held at this temperature, and it can be held for quite a long time without becoming oversaturated. The rate of reheating to 663 °C does not seem to affect the strike. Use a rate that is appropriate for your project.

After your strike hold is complete, allow the kiln to cool at its natural rate to 482 °C and begin your annealing cycle.

We recommend visually confirming that color is developing during the hold at 663 °C. If you do not see color developing, cool back down to 538 °C and hold it there for at least 4:00 before reheating to the striking range again.


Using this procedure gives you the ability to control the saturation and opalescence of cast work. Interestingly, the glass did not do anything when reheated to 593 °C or 718 °C instead of 663 °C, so the temperature range in which color strikes appears to be very narrow. If the glass is reheated to casting temperatures, it will become clear once again. If after firing it becomes necessary or desirable to re-fire the piece to casting temperature, you will need to re-strike the glass following the guidelines above.


Also of note: This glass is a little heavier than our typical glasses with a specific gravity of 2.57 g/cm3.


*If your typical casting process includes a hold at 663 °C, when cooling from process temperature to reduce the probability of "suckers," you should still do this hold. In our tests, the glass did not develop any color/opalescence when held at this temperature upon cooling from the casting temperature. It will only develop color if first cooled to 538 °C, and then reheated as described above. We have not found it necessary to repeat the slower rate of cooling used to reduce suckers after your strike hold when cooling to anneal. For additional information about suckers, see Bullseye Tip Sheet 8: Lost Wax Kilncasting.